Abstract


A weaving trial with a size-lesscotton warp yarn (20/1 Ne) was conducted under mill-like conditions on a modernhigh-speed, flexible-rapier weaving machine. About 100 yards of a 1/2-twillfabric (64 epi and up to 56 ppi - face down) was produced at speeds up to 500picks per minute with no warp yarn failure or breakage. This certainly was avery encouraging achievement, which at least demonstrated for the first timeever the "mechanical feasibility" of size-less weaving of 100% cottonyarns on a modern high-speed weaving machine. However, the quality of thefabric produced was not satisfactory, mainly because of the random formation ofunsightly, tiny fibrous balls on the fabric surface. The fuzzy ball formationmost likely was partly due to abrasion of the warp yarn (yarn-against-yarn andyarn-against-loom-components) and partly due to disintegration of the warp yarnduring weaving. The yarn disintegration probably occurred due to some loss ofyarn twist by the yarns rapid and repeated extensions and relaxations (i.e.,by the so-called yarns up-and-down dancing at a high frequency). Multi-prongefforts to eliminate the referenced fabric defects are continuing. Briefdiscussions of the weaving trial, weaving performance, and fabric quality comprisethis paper.


Introduction


According to a recent Cotton Counts& Customers publication by the National Cotton Council of America,approximately 75% of cotton produced annually worldwide is utilized in theproduction of value-added, cotton woven fabrics. This obviously makes theweaving sector of textile industry by far the largest market for cotton fiber.The weaving process almost always involves sizing or coating of warp yarns witha suitable adhesive, such as starch, polyvinyl alcohol (PVA), carboxymethylcellulose (CMC), etc.. Sizing strengthens warp yarns to withstand/combat harshmechanical stresses of weaving process and thus facilitates efficient weaving.Since the sizing ingredients, even the traces thereof, can adversely affectquality of subsequent fabric dyeing and finishing, it is imperative that thesizing chemicals are completely removed from the greige fabric at the firstopportunity, and that is done by a wet process called fabric desizing. Sinceboth warp sizing and fabric desizing are very costly, complex, andenvironmentally sensitive, the cotton textile industry obviously wants toeliminate the underlying process of warp sizing, if at all feasible. At therecommendation of National Cotton Council, the Agricultural Research Service(ARS) of the US Department of Agriculture (USDA) has directed research towardsize-free weaving. Thus, for the past 3-4 years, scientists at SouthernRegional Research Center have been conducting research investigations toexplore the possibilities of reduced sizing and, preferably, size-lessweaving (i.e., eliminating warp sizing) in the production of cotton fabrics.


About two years ago, we demonstratedthe mechanical feasibility of size-less weaving by weaving, under mill-likeconditions, about 100 yards of a relatively low-density twill fabric on aconventional (Draper) fly-shuttle loom without any warp breakage or failure.Although this was a significant milestone, the fly-shuttle loom today is almostobsolete in the American textile industry. Accordingly, the research wasredirected to use a modern high-speed weaving machine in the investigation ofsize-free weaving.


Indeed, it is a great pleasure toreport here that we now have produced, for the first time ever, withouttraditional sizing and without any yarn breakage or failure, another about 100yards of a cotton twill fabric on a modern high-speed, flexible-rapier weavingmachine operating under mill-like conditions. This certainly is a pioneeringresearch development, since no such research accomplishment in size-freeweaving of cotton fabric on modern weaving machines has ever been reported.However, in the same breath, we must also report that the fabric quality is notyet fully acceptable. Minor, nep-like (however, soft and fuzzy) balls disruptthe fabric surface. These defects most likely are caused by abrasion ordisintegration of warp yarns mostly in the reed-sweep zone. A few yards of theproduced fabric apparently do not have as many such defects, which practicallydemonstrates the feasibility of size-free weaving on a modern high-speedweaving machine. Efforts are continuing to understand the fundamentals ofsize-free weaving and to determine causes and cures of the fabric defectsencountered. This paper briefly covers what we did to achieve what we claim wehave.


 

Materials and Methods


The basic material used in the size-free weaving investigations was Acala cotton. The fiber was processed under almost mill-like conditions and spun into a 20/1 Ne (30-tex) rotor-spun yarn for both warp and filling. The yarn was warped on section beams and then beamed (assembled on a loom beam) by using different treatments on different sections of the warp. The beam was mounted on a modern high-speed, flexible-rapier weaving machine. Different reeds (viz. a conventional reed and a ceramic-coated reed), weaving speeds (varying from 250 ppm to 550 ppm), pick densities (varying from 20 ppi to 50+ ppi), and weaves (twill and plain) were investigated. A total of about 150 yards of mainly a twill fabric was produced. The Plain weaving had to be abandoned, since a weft density of even 40 ppi at 400 ppm presented difficulties. Thus, the initial weaving set-up consisted of producing a cotton twill fabric of a medium-light construction (63 x 40 ends and picks per inch, respectively) at 400 ppm. Additional weaving experiments were conducted with different weaving parameters to determine the effects of two most important weaving variables, namely, the fabric construction (cover factor/pick density) and the weaving speed, by independently varying and evaluating one variable at a time. Basically, the following is what we did to achieve what we did:


1)    Production of a cotton yarn of required structure, characteristics, quality and consistency, which would significantly contribute to attributes that are deemed desirable for size-free weaving.

2)    Development of technology to set the twist-torque or liveliness of warp yarn without traditional sizing.

3)    Modification of surface characteristics of critical components, mainly the reed, of the weaving machinery to minimize yarn abrasion and, consequently, reducing yarn breakages during size-free weaving and thereby improving weaving efficiency and fabric quality. A special ceramic-coated reed was investigated for its weaving performance

4)    Manipulation of weaving conditions and parameters, such as weaving speed, pick density, machinery settings, etc., to study their effects on the weaving performance and fabric quality. Dynamic tensions of single strands of the warp yarns were measured, using a yarn tension-cum-friction meter (See Figure 1). Hundreds of yarn and fabric photographs were captured in real time, using computer-aided techniques.





Figure 1. Single-End Dynamic Warp Tensions During Weaving


 

Results & Discussion


The 20/1 Ne (30-tex) rotor-spun yarn produced for size-free weaving evaluation had excellent metrics. For example, it had single-strand mean breaking strength of about 500 cN, count-strength product equal to 128 kN/tex, and Uster unevenness CV index of 12.8% with very low numbers of imperfections (viz., the thick and thin places and neps) at classical sensitivity levels. Incidentally, the above metrics of a rotor-spun yarn were better than those of a run-of-the-mill, ring-spun carded cotton yarn of equivalent-size. A ring-spun yarn typically is about 20% stronger than an equivalent and comparable open-end spun yarn. At any rate, the yarn performed very well with no yarn failure during warping and beaming operations.


Regarding the warp preparation for (loom) beaming, the research has shown that a continuous washing of warp sheet (under nominal tension) in boiling water (containing a wetting agent and possibly a small amount of rice soap), followed by drying (on steam-heated cylinders) can adequately relax the yarn and, hence, set/control its twist liveliness. It has also been observed that the referenced wash & dry treatment slightly increases (by ~ 15%) the yarns tensile strength, presumably due to the yarns expected shrinkage in boiling water. At any rate, the beaming process did not present an anticipated problem relating to the yarn twist torque or liveliness, which ensured that the (size-less) beaming process adopted was satisfactory. However, it may also be mentioned that, instead of the adopted, costly yarn washing and drying treatment on a dummy slasher, any other relatively less-expensive method or technique of setting the yarn twist torque (say, by using a HW Yarn Conditioner or a pressure cooker) could be deployed in conjunction with either 1) an ordinary beaming operation on a dummy slasher without heating its cylinders or 2) a modern sectional-warping process (i.e., without using a dummy slasher) to efficiently prepare a loom beam from a size-less warp. The representative scheme for beaming towards the present study is shown in Figure 2.



1)    First Treatment: No application of any fluid &/or heat.


2)    The yarn was sitting on the cylinders, while the latter were being heated from room temperature to 2200 F.


3)    Second Treatment: cylinders at 2200 F.


4)    The yarn was sitting on the cylinders at 2200 F, while the water for yarn washing was being boiled in the (size) box.


5)    Third Treatment: The yarn was washed in the boiling water and dried on the cylinders at 2200 F.


6)    Fourth Treatment: Conventional sizing


7)    The yarn was sitting on the heated cylinders, while the preparation for conventional sizing (control) was being made.


8)    Fourth Treatment: The warp was slashed with the traditional size.

 

Regarding the actual weaving performance, the mechanical aspects of the weaving process were excellent in the sense that no warp yarn breakage or failure occurred during the entire production of 150 yards of fabrics of different configurations. However, the fabric quality was not satisfactory. Noticeable pill-like, minor defects were formed on the fabric surface, which is objectionable. These fuzzy defects, as shown in Figure 3, most likely were caused by abrasion and, hence, disintegration of the warp yarns in the reed-sweep zone. Visual inspections of the fabrics showed that although some areas of the fabrics had almost negligible defects (see Figure 4), the most areas had highly significant number of those defects, which made the total fabric of unacceptable quality. Multi-directional efforts to determine the underlying cause (s) of these defects and explore possible remedies are continuing. The yarn structure, (size-less) topical treatments, specially coated loom components (especially, the reed); and weaving parameters are the primary items in the current focus.



Based on the preliminary results and observations of the size-less weaving trial conducted, it seemed that the optimum pick density (i.e., fabric construction) that could be efficiently woven, at the weaving machines commercial running speed of 500 ppm, was 40 ppi. Beyond this pick density, the weaving performance (mainly the fabric quality) at the above referenced loom speed deteriorated considerably. Even at 400 ppm, the 50 ppi density produced unsatisfactory fabric quality. In fact, a pick density greater than 50 ppi invariably produced unsatisfactory weaving results and fabric quality. However, it appeared though that the weaving speed was not as critical as the pick density. With an attainable pick density, the weaving speed did not appear to make a significant difference in the weaving performance or fabric quality. Relatively higher weaving speeds may even be attainable for relatively lower pick densities (i.e., for lighter-than-standard fabric constructions such as a medical guaze).


 

Conclusions


Actual weaving trials and related investigations conducted on a modern high-speed weaving machine have at least demonstrated the mechanical feasibility of producing cotton fabrics without the centuries-old tradition of warp sizing. To achieve efficient size-free weaving, the quality of warp yarn must be considerably superior and consistent in properties to that of the (present) run-of-the-mill type of yarn. It means that the yarn for size-free weaving must be of the highest possible uniformity and consistency and with the least amount of hairiness. Obviously, this is a function of the selected fiber quality, yarn structure, and spinning parameters. Further, a simple washing and/or drying (heating) of a cotton warp yarn seems to be adequate for preparing a loom beam without the traditional warp sizing. A ceramic-coated loom reed also appears to improve fabric quality by reducing the pill-like fuzzy defects mentioned previously. The continuing research is expected to produce new knowledge that is essential to accomplishing commercially successful size-free weaving of especially dense cotton fabrics.



References


1)    Sawhney A. P. S., et al. Preparation and weaving of cotton yarns without the traditional warp sizing: Some new concepts. Proc. Beltwide Cotton Conferences, National Cotton Council of America, Memphis, TN, January 2000.

2)    Sawhney A. P. S., et al. A successful weaving trial with a size-free cotton warp (on a fly-shuttle loom) Indian Journal of Fibers and Textile Research (IJFTR), Vol. 29, p. 117-121, June 2004.

3)    Sawhney, A. P. S., Dumitras, P.G., Sachinvala, N.D, Calamari, T.A., Bologa, M.K., and Singh, K.V. Research Approaches for reducing or eliminating warp sizing in modern high-speed weaving. American Association of Textile Chemists and Colorists (AATCC), September 2005.


Acknowledgments


The researchers duly acknowledge the National Program Staff, ARS, USDA, and the National Cotton Council of America, under whose directions and guidance the presented research was conducted. The cooperation of fellow-researchers in the Cotton Structure & Quality (CSQ) and the Cotton Chemistry and Utilization (CCU) Units at the Center is also acknowledged. Special thanks are due to Mr. Jim Sandberg and Mr. Jerome Jeanpierrs for their considerable assistance in the day-to-day research operations.


About the Authors:


The authors are associated with Southern Regional Research Center, Agricultural Research Service, USDA, New Orleans, LA.



To read more articles on Textile, Industry, Technical Textile, Dyes & Chemicals, Machinery, Fashion, Apparel, Technology, Retail, Leather, Footwear & Jewellery,  Software and General please visit https://articles.fibre2fashion.com


To promote your company, product and services via promotional article, follow this link : https://www.fibre2fashion.com/services/article-writing-service/content-promotion-services.asp